Item Details
Quarry Location:
Fatima, Ourém,Santarém District, Beira Litoral Province
Water Absorption:
3.22 %
Density:
2473 Kg/m3
Flexural Strength:
11.7- 13.3 MPa
Compressive Strength:
106.0 - 130.64 Ma
Recommended Usage:
Building stone,monuments, pool coping, sills, ornamental stone, interior, exterior, wall, floor , paving
Finishing Surface:
honed, sawn cut, brushed, tumbled, chiseled, split
Additional Names:
Filstone Beige MV,Filstone Beije MV
Description:
Apparent density measurement 2473,00 Kg/m3
Open porosity measurement 8,45 %
Water absorption measurement at normal atmospheric press. 3,22 %
Capillary water absorption 12,55 g/m2. s0.5
Uniaxial compressive strength in dry conditions 130,64 MPa
Uniaxial compressive strenght after freeze/thaw test 106,00 MPa
Flexural strength under central load in dry conditions 13,30 MPa
Flexural strength under central load after freeze/thaw test 11,70 MPa
Flexural strength under central load after thermal shock 12,00 MPa
Percentage of volume change after frost cycles 29,00% (140 cycles)
Breaking load at dowel hole 2041,67 N
Sound speed propagation ( Pulse velocity ) 5,05 km/s
Rupture energy 3,00 J
Abrasion resistance 22,25 mm
Slip resistance in dry conditions - sawn (coefficient of friction*100) 55,83